Every sign of failure the Technical Library records under Superstructure: 32 signs across 4 elements and spaces. Each row gives what you see, the likely cause and what confirms it, and the next step. Each heading opens the page the rows come from.

Load-Bearing Masonry

Restraint, bowing and rubble cores

What you seeLikely cause, and what confirms itNext step
Wall bowing outward with floors running parallelLack of restraint. Plumb survey; inspection of floor-to-wall connections.Tie the wall to the floors and roof with straps, tie rods or helical ties; prop it meanwhile.
Bulging stone face with cracksSeparation from the rubble core. Tapping; endoscope into the core.Grout the rubble core and pin the stone face, or rebuild badly bulged sections.

Alterations, overload and lintels

What you seeLikely cause, and what confirms itNext step
Cracks below the ends of a new beamInadequate bearing or padstone. Opening up at the bearing.Open up the bearing; add a padstone or spreader beam.
Dropped brickwork over an openingFailed lintel or spreading arch. Inspection of lintel or abutment.Prop the opening; replace the lintel or repair the arch.
Vertical cracks in a heavily loaded pierOverload or crushing. Load review.Review the loads with an engineer; relieve or strengthen the pier.
Masonry building being extended upward or converted to flatsA change of consequence class. In England, flats and offices of more than 4 and up to 15 storeys fall in Class 2b, which needs horizontal and vertical ties or a check that the loss of any one wall does not cause disproportionate collapse (Approved Document A, Table 11).Have the robustness assessed before the change, and add ties or strengthening where the new class requires it.

Earthquake and settlement

What you seeLikely cause, and what confirms itNext step
Diagonal cracks through openingsFoundation movement. See the foundations page.Treat it as foundation movement; see Foundations.
Cracks wider at one end and opening over monthsProgressive movement. Crack monitoring, with widths graded on the asset’s market’s damage scale (Thresholds by market).Monitor and find the cause before repair; have an engineer assess cracks in the moderate band or above.

Structural Core

Openings and removed bracing

What you seeLikely cause, and what confirms itNext step
Many cores and openings through a lift coreAccumulated service penetrations. Survey against drawings; engineering review.Survey against the drawings; get an engineering review, with strengthening around openings where needed.
Warehouse bay without the bracing shown on drawingsBracing removed for doors or racking. Drawing comparison.Install temporary bracing now; reinstate or relocate it to an engineer's design.
Building now taller or more public than its original classRobustness short of the new consequence class. In England offices and flats over 15 storeys fall in Class 3 and need a systematic risk assessment, while those over 4 storeys sit in Class 2b (Approved Document A, Table 11).Have the lateral system and robustness assessed before the change.

Soft storeys, cracking and movement

What you seeLikely cause, and what confirms itNext step
Diagonal cracks in a shear wallShear distress from overload, settlement or past earthquake. Engineering assessment.Get an engineering assessment, then repair or strengthen.
Noticeable sway in windReduced stiffness or design limits. Monitoring; assessment.Monitor the sway, and have it assessed.
Rust staining or spalling on concrete core wallsReinforcement corrosion. Carbonation depth and chloride at bar depth: the carbonation front marks a fall in pH from about 12.5 to 8.5, shown by phenolphthalein on a fresh break, and the chloride threshold is generally taken as 0.2 to 0.4 per cent by mass of cement (Institute of Corrosion).Map the corrosion, repair the concrete, and protect it against further carbonation or chloride.

Connections and construction defects

What you seeLikely cause, and what confirms itNext step
Slack or bent bracing rodsMovement, impact or corrosion. Inspection.Inspect, then retension, repair or replace the rods and their connections.
Lift doors binding or guide rails out of lineCore movement or settlement. Verticality survey of the core; the lift contractor’s alignment records.Survey the core and have an engineer review it before the lift is realigned.

Structural Frame

Carbonation and chlorides

What you seeLikely cause, and what confirms itNext step
Cracking and spalling along bars across a facade or soffitCarbonation-induced corrosion. Carbonation depth at the steel; low cover. The carbonation front marks a fall in pH from about 12.5 to 8.5, shown by phenolphthalein on a fresh break (Institute of Corrosion).Patch repair, then anti-carbonation coatings or realkalisation.
Localised spalling in a car park, especially near joints and drainsChloride-induced corrosion. Chloride content at bar depth, against a threshold generally taken as 0.2 to 0.4 per cent by mass of cement (Institute of Corrosion); half-cell potentials.Repair with cathodic protection, and fix the deck drainage and membranes.

Alkali-silica reaction and problem concretes

What you seeLikely cause, and what confirms itNext step
Map cracking with white gelAlkali-silica reaction. Petrographic examination of cores.Confirm by petrographic examination; have an engineer assess, and strengthen where needed.

Punching shear and alterations

What you seeLikely cause, and what confirms itNext step
Cracking around columns on the top of a flat slabPunching shear distress. Engineering assessment; deflection survey.Call an engineer urgently; prop if advised, restrict loads, and add punching shear reinforcement.
Diagonal cracks near beam supportsShear distress. Engineering assessment.Get an engineering assessment; strengthen with plates, wraps or added members.
Vertical cracks at mid-span soffitsFlexural cracking from load or loss of capacity. Load review against the design loads and the asset’s market (Thresholds by market); reinforcement check.Review the loads and check the reinforcement; restrict loads or strengthen.
Beams or slabs visibly sagging, with cracked partitionsDeflection beyond serviceability. Level survey against the design limits and the asset’s market (Thresholds by market).Survey the deflection, compare it with the design, and have an engineer advise on loads or strengthening.

Steel corrosion and fire damage

What you seeLikely cause, and what confirms itNext step
Rust bleeding through masonry at column linesEncased steel corrosion. Opening up.Open up, treat and recoat the encased steel, or replace badly corroded members.

Upper Floor Slabs & Structures

Deflection, overload and vibration

What you seeLikely cause, and what confirms itNext step
Sagging mid-span and cracked partitions belowCreep deflection or overload. Level survey and load review, against the asset’s market (Thresholds by market).Survey the levels and review the loads; restrict loads or strengthen.
Cracks under heavy storage areasOverload. Loads against design.Move heavy items over beams and columns, limit storage, and post load notices.
Lively floor under footfallLow stiffness and mass. Vibration measurement.Measure the vibration; add stiffness or mass.
Partitions cracking along their head on an upper floorSlab deflection after the partitions were built. Deflection since the partitions went in, against span/500, or 20 mm for brittle finishes (The Structural Engineer).Fit deflection heads to the partitions, and have the slab assessed if movement continues.
Heavy plant, compactus or stock on an existing floorLoads beyond the design imposed load. Load review against the design loads, the floor’s capacity and the asset’s market (Thresholds by market).Move heavy items over beams and columns, spread the load, or strengthen the floor, and post load notices.

Post-tensioning, precast and decking

What you seeLikely cause, and what confirms itNext step
Broken concrete around a cored holeTendon or reinforcement cut. Scanning; drawings.Scan and check the drawings; get specialist repair if a tendon has been cut.
Rust staining on decking soffitsWater through the slab above. Leak source above.Stop the leak above, then repair the decking.

Timber floors

What you seeLikely cause, and what confirms itNext step
Springy timber floorUndersized joists, lost strutting, or notching. Inspection.Sister or replace joists, restore strutting, and repair bearings.